Flotation performance of a de-slimed(-150+53μm)Jordanian siliceous phosphate was evaluated in a batch laboratory flotation column 100 cm high and 5 cm inside diameter.The collector used during anionic flotation wa...Flotation performance of a de-slimed(-150+53μm)Jordanian siliceous phosphate was evaluated in a batch laboratory flotation column 100 cm high and 5 cm inside diameter.The collector used during anionic flotation was sodium oleate while an amine acetate(AEROMINE 3100C)was used for cationic flotation.Flotation comparison at different collector dosage,superficial gas velocity,and frother concentration showed that the maximum difference in performance between cationic and anionic flotation was obtained with these flotation parameters:30×10^(-6)(mg/L)frother concentration,250 g/t collector concentration,and 3.4 cm/s superficial gas velocity.At these operating conditions amine (cationic)flotation gave 7%higher flotation recovery,a 6%cleaner concentrate grade,and was 6%more efficient at removing silica.展开更多
Selective separation of silica from a siliceous-calcareous phosphate ore that had been sieved into different size fractions is investigated by a combination of chemical analysis,zeta potential measurement and FTIR and...Selective separation of silica from a siliceous-calcareous phosphate ore that had been sieved into different size fractions is investigated by a combination of chemical analysis,zeta potential measurement and FTIR and XPS techniques.Scrubbing is a better choice than flotation for removing silica from the coarse fractions.The P_2O_5 grade of the coarse fractions is increased to about 30%by scrubbing and the product yields are higher than those obtained by flotation.The silica in the fine fraction is separated by reverse flotation.An alkyl amine salt(DAH)is an effective collector and the P_2O_5 grade of the fine fraction can be increased by 7%to beyond 30%under acidic conditions.The higher zeta potential obtained using DAH suggests that it is more strongly absorbed onto the ore particles than the other cationic collectors. FTIR and XPS results confirm physical absorption of the cationic collector onto the ore surface.They also indicate that calcite is dissolved at low pH values,which increases the Si concentration on the ore surface.展开更多
基金done during the first author's Fulbright fellowship at the Center for Advanced Separation (CAST)/Virginia Technical Institute and State University-USA. Salah would like to thank all the people who work at CAST for their friendship and support during his stay in Blacksburg, VA.
文摘Flotation performance of a de-slimed(-150+53μm)Jordanian siliceous phosphate was evaluated in a batch laboratory flotation column 100 cm high and 5 cm inside diameter.The collector used during anionic flotation was sodium oleate while an amine acetate(AEROMINE 3100C)was used for cationic flotation.Flotation comparison at different collector dosage,superficial gas velocity,and frother concentration showed that the maximum difference in performance between cationic and anionic flotation was obtained with these flotation parameters:30×10^(-6)(mg/L)frother concentration,250 g/t collector concentration,and 3.4 cm/s superficial gas velocity.At these operating conditions amine (cationic)flotation gave 7%higher flotation recovery,a 6%cleaner concentrate grade,and was 6%more efficient at removing silica.
基金the National Key Technology R&D Program of China forthe support of this work(No.2007BAE58B01).
文摘Selective separation of silica from a siliceous-calcareous phosphate ore that had been sieved into different size fractions is investigated by a combination of chemical analysis,zeta potential measurement and FTIR and XPS techniques.Scrubbing is a better choice than flotation for removing silica from the coarse fractions.The P_2O_5 grade of the coarse fractions is increased to about 30%by scrubbing and the product yields are higher than those obtained by flotation.The silica in the fine fraction is separated by reverse flotation.An alkyl amine salt(DAH)is an effective collector and the P_2O_5 grade of the fine fraction can be increased by 7%to beyond 30%under acidic conditions.The higher zeta potential obtained using DAH suggests that it is more strongly absorbed onto the ore particles than the other cationic collectors. FTIR and XPS results confirm physical absorption of the cationic collector onto the ore surface.They also indicate that calcite is dissolved at low pH values,which increases the Si concentration on the ore surface.